Dec 07, 2023 Leave a message

Silicon Barium Alloy in Steel Smelting: Deoxidation and Inclusion Control

Why Deoxidation Determines Steel Cleanliness

Oxygen dissolves readily in liquid steel and remains in solution until the steel freezes, when it is rejected as carbon monoxide or as oxide inclusions. Those inclusions are the origin of many downstream defects: blowholes and pinholes in the ingot, surface seams in the billet, fatigue initiation sites in finished parts, and clogged submerged entry nozzles in continuous casting. Deoxidation is therefore not a finishing step but a core part of steelmaking practice.

The workhorse deoxidizer is aluminium, because it is cheap and powerful. Its drawback is that the reaction product, solid alumina, forms hard angular clusters that are difficult to float out of the bath. Silicon barium alloys and silicon calcium barium alloys were developed to combine strong deoxidizing power with a reaction product that stays liquid and can be removed with the slag.

Composition and Function of Silicon Barium Alloys

Silicon barium and silicon calcium barium alloys are ferroalloy products whose active elements are silicon, barium and, in the calcium-bearing grades, calcium. Silicon supplies most of the deoxidizing capacity by mass, while barium and calcium act on the residual oxygen and on the shape of the inclusions that remain.

Product Si Ba Ca Al Typical size
Silicon barium alloy 55-65 % 8-15 % - max 2.0 % 10-50 mm, or 0-2 mm powder for cored wire
Silicon calcium barium alloy, high calcium 50-60 % 8-12 % 8-12 % max 1.5 % 10-50 mm, or 0-2 mm powder for cored wire
Silicon calcium barium alloy, medium calcium 45-55 % 5-10 % 5-10 % max 1.5 % 10-60 mm, or 0-2 mm powder for cored wire

Barium is the element that makes these alloys distinctive. Calcium boils at about 1484 C, which is below normal steelmaking temperatures, so a large part of any calcium addition is lost as vapour before it can react. Barium has a much higher boiling point and lowers the activity of calcium in the alloy, so more of the calcium dissolves in the steel and does useful work instead of fuming off at the ladle surface.

The Reaction Sequence in the Ladle

When a silicon barium or silicon calcium barium alloy is fed into a ladle, the elements react in a known order because their affinity for oxygen differs.

Silicon reacts with dissolved oxygen to form silica, lowering the oxygen content of the bath quickly and providing the bulk of the deoxidizing effect.

Barium follows, reacting with the remaining oxygen and contributing to desulphurization as barium sulphide.

Calcium reacts with any residual oxygen and, more importantly, with existing solid alumina inclusions, converting them into liquid calcium aluminates.

The liquid reaction products coalesce, grow and float into the slag, where they are absorbed and removed from the steel.

The practical consequence of this sequence is that oxygen is removed in two stages: first a bulk drop by silicon, then a final cleanup by barium and calcium. The result is a lower total oxygen content and a lower inclusion count than silicon alone can deliver.

Inclusion Modification and Sulphide Shape Control

Solid alumina inclusions are the most damaging residue of aluminium deoxidation. Calcium converts them to calcium aluminates that are liquid at steelmaking temperature, so they coalesce into larger globules and rise faster. Residual globules that stay in the steel are softer and less harmful than angular alumina, which improves fatigue life in rail steel, bearing steel and other demanding products.

Sulphur behaves in a similar way. In untreated steel, sulphur forms manganese sulphide that is deformed into long stringers during rolling, creating planes of weakness and anisotropy in properties. Calcium and barium combine with sulphur to form sulphides that remain globular and undeformed, so the steel retains more uniform transverse properties. This is why silicon calcium barium alloys are common in rail steel, where transverse ductility and toughness are critical, and in stainless and special steels where inclusion control supports corrosion resistance and machinability.

Feeding Practice and Recovery

The alloy is normally added in one of two ways. Lumpy material is thrown into the ladle during tapping, where it dissolves in the falling metal stream. Powder blended into steel or aluminium cored wire is injected deep into the ladle after tapping, which gives better control and higher recovery.

Addition rate. Typical levels are 1.0-2.5 kg per tonne of steel, adjusted from the oxygen content measured after primary deoxidation.

Recovery. Calcium recovery in wire injection commonly falls in the range 30-50 %, because some calcium always vaporises. Barium and silicon recoveries are higher.

Timing. Treat after slag deoxidation, with a killed bath and a fluid slag, so that reaction products can be absorbed rather than suspended.

Stirring. Gentle argon stirring for several minutes after the addition helps the liquid inclusions float out; violent stirring entrains slag and defeats the purpose.

Frequently Asked Questions

Q: What is the difference between silicon barium and silicon calcium barium?
Silicon barium contains silicon and barium only and is used where strong deoxidation and desulphurization are needed without adding calcium. Silicon calcium barium also carries calcium, which modifies solid alumina inclusions into liquid aluminates, so it is chosen when inclusion control and sulphide shape control are required.

Q: Why is barium effective when calcium alone is not?
Calcium boils below steelmaking temperature and is largely lost as vapour. Barium raises the boiling point of the alloy system and lowers calcium activity, so a larger share of the calcium dissolves in the steel and reacts with inclusions before it can escape.

Q: Can these alloys replace aluminium deoxidation entirely?
In many special steel grades they can, and in grades where aluminium is restricted they are the preferred route. In plain carbon steels aluminium remains more economical, and the barium or calcium bearing alloy is then used as a final inclusion treatment rather than as the primary deoxidizer.

Q: How is the alloy composition verified?
Chemical analysis is normally carried out by the methods of the GB/T 223 series for steel and alloy analysis, or by optical emission spectrometry after dissolution of a representative sample. Size distribution and powder density are checked separately for cored wire applications.

Q: What causes poor recovery of calcium?
Late addition into a shallow ladle, a thick oxidised slag, no stirring after injection, and excessive argon flow that exposes the bath surface are the usual causes. Deep injection with a properly designed lance and controlled stirring gives the most consistent results.

Q: Is moisture a problem with these alloys?
Yes. Silicon barium and silicon calcium barium products should be stored dry, because absorbed moisture introduces hydrogen into the steel and can cause porosity in the finished product. Bags should stay sealed until the moment of use.

Send Inquiry

Home

Phone

E-mail

Inquiry