The test material is TC4 titanium alloy bar hot rolled at 920°C. The total deformation rate of hot rolling is about 80%, and the a+β/β phase transformation point is 980~990°C. The samples were heated and kept at 1000°C, 950°C, 930°C, and 830°C for 1 hour and then air-cooled, water-cooled, and furnace-cooled respectively. Different annealing methods have an impact on the microstructure and mechanical properties.

info-800-533

The cooling rate has a great influence on the microstructure and mechanical properties of the above four temperatures. When water-cooled, the β-phase components in equilibrium at 1000°C, 950°C and 930°C will all undergo martensite transformation, and the β-phase transforms into martensite a` needles. It shows an obvious Widmansite structure at 1000°C, and its mechanical properties are equivalent to those of air cooling at 1000°C. On the water-cooled samples at 950°C and 930°C, the microstructure has similar characteristics to that of air cooling, but there are β+ martensite a` needles between the equiaxed primary a phases. At this time, the corresponding comprehensive performance is the highest, and it has better creep resistance than the air-cooled structure.

 

info-800-533

 

When kept at 830°C, the balanced β phase components no longer touch the M line, but after water cooling, very small needle-like transformation products are also found in the intergranular β phase, which can only be distinguished with an electron microscope. However, the structure of the needle-like product has not yet been determined. At this time, the tensile strength and area reduction are very low. As for the furnace cooling, due to the slow cooling rate of the sample and the long residence time at high temperature, the polymorphic transformation is fully carried out and all the a phases become coarse. After furnace cooling at 1000°C, coarse a-phase flakes and inter-flake β-phases are produced in the original β-grains, and there is also a thick network of strip-like a-phases on the original β-grain boundaries, which is generally called a basket-like structure. After furnace cooling at 950°C, 930°C and 830°C, since the a phase tends to nucleate and grow at the original a phase interface, the microstructure is all equiaxed a and intergranular β phases. The tensile strength after furnace cooling at 1000°C is lower than that of air cooling and water cooling, and the tensile plasticity is higher. The comprehensive performance after furnace cooling at other temperatures is also lower than that of water cooling and air cooling.

info-800-533
In summary, in order to obtain the best comprehensive strength and plasticity properties of TC4 titanium alloy, as well as good creep resistance and fracture toughness, an annealing process of air cooling (or water cooling) after holding at 950°C for 1 hour can be used. In order to facilitate subsequent processing, when the metallurgical factory leaves the factory, TC4 titanium alloy adopts the process of air cooling at 700~800℃ for 1 hour. For some large-size forgings, in order to ensure the uniformity of performance, the furnace cooling process is sometimes used.