Jan 16, 2024 Leave a message

How To Deal With Excessive Slag In The Furnace?

Reasons for excessive slag in the furnace:
1. Sometimes there is a long-term lack of carbon in the furnace, and a large amount of excess silica melts to form sticky slag, which is difficult to remove.


2. Due to reasons such as high material surface, the depth of electrode insertion into the furnace material becomes shallow, the furnace temperature is low, and the slag is difficult to remove. Especially in electric furnaces with small capacities, this phenomenon is more likely to occur, causing too much slag to accumulate in the furnace.


3. Although the amount of slag is small when smelting ferrosilicon, the slag should be taken out as much as possible when tapping to allow the electrode to be inserted deeply. If you don't pay attention to the slag, over time, there will be too much slag in the furnace.


4. Poor raw material quality, such as excessive ash content in coke or excessive soil on the surface of silica, will also increase the amount of slag.

news-700-466
The dangers of too much slag in the furnace:
1. The bottom of the furnace rises, making it difficult for the click to be inserted deeply, shrinking due to drying, deteriorating the air permeability of the material surface, and worsening the furnace condition.


2. The furnace bottom temperature is low, the tap hole is difficult to open, the tap hole is not smooth, the flow rate of molten iron is slow, and the tap volume is small.

 

news-700-466
How to deal with excessive slag in the furnace:


1. For large-capacity furnaces, you can add 200 to 300 kilograms of lime blocks to the electrode surface of the taphole phase or add 100 to 200 kilograms of fluorspar half an hour before tapping to dilute the slag. Smaller-capacity electric furnaces can add 30 to 40 kilograms of steel chips to facilitate slag removal.

 

2. The tap should be adapted to take as much slag out as possible. The electric furnace with a small capacity can also appropriately expand the tap hole to facilitate inspection.

 

3. Handle the furnace conditions well, insert the electrode deeply and increase the furnace temperature.

 

4. Coke with lower ash content should be used as much as possible. If conditions permit, the silica should be washed with water to reduce the factor of slag generation in the furnace.

news-700-466

Send Inquiry