The effect of carboniser particle size. The absorption rate of the carburant depends on the combined effect of the dissolution and diffusion rate of the carburant and the oxidative loss rate: in general, the carburant particles are small, the dissolution rate is fast, and the loss rate is large; the carburant particle size is large, the dissolution rate is slow, and the loss rate is small. Selection of the size of the carburant is related to the diameter and capacity of the heating furnace. Generally speaking, the diameter and capacity of the heating furnace, the size of the carburant to be larger; on the contrary, the size of the carbonising agent will be smaller.

The effect of the amount of carbon enhancer added, at a certain temperature and the same chemical composition, the saturation concentration of carbon in the iron solution is constant. Under a certain degree of saturation, the more carboniser is added, the longer the time required for dissolution and diffusion, the greater the corresponding loss and the lower the absorption rate.

The effect of temperature on the absorption rate of the carboniser. From the kinetic and thermodynamic point of view, the oxidation of iron solution is related to the equilibrium temperature of the C-Si-O system, i.e., O in the iron solution will react with C and Si. The equilibrium temperature varies with the target carbon and silicon content. When the iron solution is above the equilibrium temperature, carbon is preferentially oxidised and CO and CO2 are formed from C and O. Consequently, there is an increase in the oxidative loss of carbon from the iron solution. As a result, the uptake of carbon increment decreases when the equilibrium temperature is higher than the equilibrium temperature. When the carbon increment temperature is lower than the equilibrium temperature, the saturation solubility of carbon decreases, while the rate of carbon dissolution and diffusion decreases, and the yield also decreases. At the equilibrium temperature, the absorption rate of the carbon enhancer is high.

The effect of ferrofluid stirring on the absorption rate of the carbon enhancer. Stirring is conducive to the dissolution and diffusion of carbon, avoiding the carbonizer floating on the iron surface due to combustion. Before the carboniser is completely dissolved, the stirring time is long and the absorption rate is high. Stirring can also reduce the carbonation and holding time, shorten the production cycle, and avoid the burning of alloying elements in the iron solution. However, too long stirring time not only has a great impact on the service life of the furnace, but also in the solution with carboniser, stirring will increase the loss of carbon in the iron solution. Therefore, the appropriate stirring time of the iron solution should ensure the complete dissolution of the carbonating agent.

The influence of the chemical composition of the iron solution on the absorption rate of the carboniser. When the initial carbon content of the ferro solution is high, under a certain dissolution limit, the absorption rate of the carbon enhancer is slower, the absorption is smaller, the combustion loss is larger, and the absorption rate of the carbon enhancer is lower. When the initial carbon content of the iron is low, the opposite is true. In addition, silicon and sulfur in the iron solution will hinder the absorption of carbon and reduce the absorption rate of the carbon enhancer. Manganese helps carbon absorption and increases the absorption rate of the carbon enhancer. In terms of the degree of influence, the influence of silicon is large, followed by manganese, and the influence of carbon and sulfur is small. Therefore, in the actual production process, manganese should be increased first, then carbon, then silicon.