Jan 31, 2024 Leave a message

Melting and Casting of Titanium Alloys: Arc Melting, Vacuum Arc Remelting and Skull Melting

Titanium and its alloys cannot be melted in contact with ordinary refractory linings. At melting temperature the metal reduces most oxides, and it absorbs oxygen, nitrogen, hydrogen and carbon readily, which embrittles the alloy. This is why titanium melting is carried out under vacuum or under high-purity inert gas in a water-cooled copper crucible, where a thin solidified layer of the alloy itself acts as the container wall.

Why Titanium Melting Needs Vacuum or Inert Gas

The melting point of commercially pure titanium is 1668 deg C, and Ti-6Al-4V, the most widely used alloy, is melted in the same range. At those temperatures the liquid metal is highly reactive: oxygen and nitrogen raise hardness and reduce ductility, hydrogen causes porosity, and carbon forms hard inclusions. A refractory crucible would contaminate the melt while being eroded by it, so the melt is contained either by a water-cooled copper hearth or by a self-generated solid shell of the same alloy.

For reference, the chemical requirements of the standard wrought Grade 5 (Ti-6Al-4V) composition under ASTM B348 are aluminium 5.5 to 6.75%, vanadium 3.5 to 4.5%, iron 0.30% maximum, oxygen 0.20% maximum, carbon 0.08% maximum, nitrogen 0.05% maximum and hydrogen 0.015% maximum. Those interstitial limits are the reason melting practice is judged on contamination control rather than on throughput alone.

Route 1 - Non-Consumable Electrode Arc Melting

In this route an electric arc is struck between a non-consumable electrode, usually tungsten or graphite, and the charge under vacuum or inert gas protection. The charge sits in a water-cooled copper hearth or crucible and is melted by the arc, then solidified. The process is flexible in charge composition and is often used to prepare electrodes for the subsequent remelting step, to melt scrap and revert material, or to produce small heats and experimental alloys where a full electrode cannot be justified.

The limitations are contamination from the electrode itself and the relatively small melt size. Graphite electrodes can add carbon, while tungsten electrodes must be positioned so that they cannot enter the melt pool.

Route 2 - Vacuum Arc Remelting in a Water-Cooled Copper Crucible

Vacuum arc remelting uses a consumable electrode made from compacted and welded titanium or titanium alloy as the cathode and a water-cooled copper crucible as the anode. The arc melts the tip of the electrode, and the metal falls as droplets into the molten pool below. The pool surface is kept liquid by the arc, while the metal in contact with the crucible wall and the base is forced to cool, so solidification proceeds from the bottom upwards.

The result is a directionally solidified ingot with a relatively sound structure and low gas content. Segregation control, arc stability and the melt rate are the key operating variables, and the electrode must be straight, correctly welded and free of volatile contamination for the arc to remain stable through the whole melt.

Route 3 - Skull Melting with a Condensation Shell

Skull melting takes the water-cooled crucible principle one step further. Between the copper crucible and the liquid alloy there is a thin solid shell of the same titanium alloy, known as the skull or condensation shell. Because the shell is made of the same material as the melt, it acts as the crucible lining and prevents contamination of the liquid titanium by the copper wall.

This configuration can be combined with centrifugal pouring to cast shaped parts, which is why it is used for investment-cast and shaped castings. The melt is held in a skull within the crucible, then poured or centrifugally thrown into the mould. After pouring, the layer of skull left behind remains in place and continues to serve as the lining for the next heat, which reduces both contamination risk and crucible consumption. The arrangement also makes the process well suited to repeated small and medium heats of the same alloy.

Casting, Solidification and Inspection Controls

Control point Objective
Chamber atmosphere vacuum or high-purity inert gas to keep oxygen and nitrogen out of the melt
Charge cleanliness no oil, moisture, paint or mixed scrap that would add hydrogen and interstitials
Pour temperature sufficient superheat for mould filling without excessive shrinkage porosity
Mould condition clean, correctly baked shell or die lining to avoid gas defects
Chemistry check analysis of the finished cast or ingot against the specified grade
Non-destructive testing radiography and dye penetrant examination of the cast surface and internal soundness
Heat treatment stress relief or annealing per the applicable product specification

Casting specifications follow the product form. ASTM B367 covers titanium castings, including Grade C-5 for Ti-6Al-4V, while wrought product is ordered to specifications such as ASTM B348. Cast components are frequently accepted on a combination of chemical analysis, radiographic soundness and mechanical testing from a coupon cast with the production lot.

Frequently Asked Questions

Q: Why can titanium not be melted in a refractory crucible?
A: Liquid titanium reduces most refractory oxides and absorbs oxygen and nitrogen, which embrittles the alloy. Melting is therefore done in water-cooled copper or in a skull of the same alloy.

Q: What is the difference between non-consumable arc melting and vacuum arc remelting?
A: Non-consumable arc melting uses a tungsten or graphite electrode and is flexible for small heats and electrode preparation. Vacuum arc remelting uses a consumable electrode of the alloy itself and produces a directionally solidified ingot with better homogeneity.

Q: What is the condensation shell in skull melting?
A: It is a thin solid layer of the same alloy that forms between the water-cooled copper crucible and the liquid melt. It protects the melt from copper contamination and remains in the crucible as the lining for the next heat.

Q: Which interstitial elements are controlled during melting?
A: Oxygen, nitrogen, hydrogen and carbon. In wrought Ti-6Al-4V to ASTM B348 the limits are 0.20% oxygen, 0.05% nitrogen, 0.015% hydrogen and 0.08% carbon as maxima.

Q: Which standard applies to Ti-6Al-4V castings?
A: ASTM B367 covers titanium castings and includes Grade C-5 for Ti-6Al-4V. Wrought bar product is ordered to standards such as ASTM B348.

Q: How is casting quality verified?
A: By chemical analysis of the finished part, radiographic examination for internal soundness, dye penetrant inspection of surfaces, and mechanical testing of coupons cast with the same lot.

Send Inquiry

Home

Phone

E-mail

Inquiry