Titanium as a Corrosion-Resistant Construction Material
Titanium is specified in chemical plants because of one self-renewing property: in air or in any oxygen-bearing medium it instantly grows a thin, coherent oxide film, only a few nanometres thick, that is chemically inert and mechanically stable. If the film is scratched or abraded during fabrication the oxide reforms within milliseconds, so the metal stays passive even where the surface has been damaged. That film is insoluble in chloride solutions, which is why titanium resists pitting, crevice attack and chloride stress-corrosion cracking far better than the austenitic stainless steels used in the same circuits.
Commercially pure titanium has a density of about 4.51 g/cm3 and melts at 1668 °C. Its modulus of elasticity, close to 105 GPa, is roughly half that of carbon steel, and its thermal conductivity is markedly lower than that of either carbon steel or stainless steel. Both values shape equipment design: shells and tube bundles need closer support spacing, and differential expansion against steel or cast iron has to be absorbed by flexible elements or sliding supports rather than restrained.
The workhorse grades for chemical service are the unalloyed grades, Grade 1 and Grade 2, known as TA1 and TA2 in GB/T 3620.1 and supplied as plate, sheet and strip to ASTM B265. Where a reducing medium or a hotter brine is involved, the alloyed grades Grade 7 and Grade 12, modified with small palladium or nickel-molybdenum additions, are chosen instead. Grade 2 covers the great majority of oxidising and neutral duties; the alloyed grades extend the useful range where unalloyed titanium would be attacked.
Why Titanium Outperforms Stainless Steel in Chloride Media
Chloride ions are the classic enemy of stainless steel. Even the molybdenum-bearing austenitic grades can suffer pitting, crevice corrosion and, under tensile stress at moderate temperature, chloride stress-corrosion cracking. Titanium behaves differently. Its passive film is stable in neutral and acidic chloride solutions, in wet chlorine, in hypochlorite and in chlorine dioxide, so equipment that would need frequent replacement in 316L can run for many years in titanium.
The practical boundary is the chemistry of the medium. Titanium performs well in oxidising acids, including nitric acid, and in most chloride brines. In strongly reducing acids such as hydrochloric or dilute sulphuric acid the film cannot repair itself and corrosion proceeds, which is exactly the situation the palladium-modified and nickel-molybdenum grades were developed for. Media containing fluoride ions, and hydrofluoric acid in particular, attack titanium aggressively and must be excluded from the process side. Hydrogen pickup, or hydriding, is the other limit: in reducing conditions above roughly 80 °C, atomic hydrogen can diffuse into the metal and embrittle it, so service temperature and chemistry have to be assessed together.
Applications in the Chlor-Alkali Industry
The chlor-alkali industry is a basic raw-material industry, and its output directly influences a wide range of downstream manufacturing. Its process streams are unusually aggressive because they combine concentrated chloride brines with wet chlorine and hypochlorite. Titanium's resistance to chloride ions is superior to that of the common stainless steels and most non-ferrous metals, which is why it has become the standard material for metal anode electrolysers, ion-exchange membrane electrolysers, wet chlorine coolers, refined brine preheaters, dechlorination towers and chlorine cooling and washing towers.
Historically the main components of this equipment were built from non-metallic materials such as graphite and polyvinyl chloride. Those materials have poor mechanical strength, poor thermal stability and poor processing behaviour, so the resulting equipment was bulky, energy-intensive and short-lived, and it often degraded product quality or introduced contamination into the process. Titanium components are thinner, stronger, thermally stable and immune to the chloride attack that limits all of those alternatives.
Applications in the Soda Ash Industry
Soda ash is one of the fundamental chemical raw materials and is tied directly to the development of the wider economy. In soda ash production the gas media are predominantly ammonia and carbon dioxide, while the liquid media are concentrated sodium chloride, ammonium chloride, ammonium bicarbonate and chloride-bearing solutions. Under those conditions carbon steel and cast iron corrode rapidly.
The consequences are visible in the main equipment items: carbonisation tower tubes, hot mother liquor coolers, crystalliser external coolers and similar exchangers built from carbon steel or cast iron suffer serious corrosion leakage and typically have a service life of no more than three years. Replacing those wetted parts with titanium removes the corrosion mechanism, cuts unplanned shutdowns and keeps the process liquor free of iron contamination, which in turn protects product purity.
Selection, Fabrication and Design Practice
Titanium is normally selected on the basis of the actual process chemistry rather than on a generic corrosion table, because small changes in temperature, aeration, pH or fluoride content can change the answer. The table below summarises the usual starting point for the main equipment groups.
| Equipment | Dominant medium | Usual titanium grade | Reason for selection |
|---|---|---|---|
| Membrane and metal anode electrolysers | Concentrated brine, wet chlorine | Grade 2 | Immunity to chloride pitting and crevice attack |
| Wet chlorine coolers | Wet chlorine, hypochlorite | Grade 2 | Stable passive film in oxidising chlorine media |
| Brine preheaters | Refined brine at elevated temperature | Grade 2 or Grade 12 | Retained passivity at higher temperature |
| Dechlorination and washing towers | Chloride, hypochlorite, traces of acid | Grade 2 | Long life compared with graphite and plastics |
| Carbonisation tower tubes and coolers | Ammonia, carbon dioxide, chloride liquors | Grade 2 or Grade 7 | Replaces carbon steel with a service life under three years |
Fabrication rules matter as much as grade selection. Titanium is welded under inert gas shielding with a trailing shield to protect the hot metal until it cools below the oxidation threshold, and the work area is kept free of iron contamination from carbon steel tools, jigs and grinding debris, since embedded iron particles become sites for localised attack. A nitric-hydrofluoric pickle is used only as a controlled surface treatment after welding and is always followed by thorough rinsing, because residual fluoride is precisely the species that destroys titanium's passivity. Minimum wall thicknesses are set by stiffness and by allowable deflection rather than by corrosion allowance, and dissimilar joints with steel or nickel alloys need insulating or transition arrangements to avoid galvanic effects.
Frequently Asked Questions
Q: Can titanium be used with hydrochloric or sulphuric acid?
Only with care. Unalloyed grades are limited to dilute or aerated conditions at low temperature. Grade 7, modified with palladium, and Grade 12, modified with nickel and molybdenum, are the correct choices for reducing acids, and the specific concentration and temperature pair must be confirmed against corrosion data before the equipment is ordered.
Q: What is the maximum service temperature for titanium equipment?
In dry oxidising service titanium components are used at several hundred degrees Celsius. In wet chemical service the limit is set by the medium rather than by the metal, because hydrogen pickup in reducing conditions becomes significant above roughly 80 °C. Temperature and chemistry therefore have to be evaluated as a pair.
Q: How is titanium welded without losing corrosion resistance?
Tungsten inert gas welding with full inert gas shielding of the weld pool, the trailing weld and the back side is standard. The heat tint that forms if shielding is lost must be removed mechanically or by pickling, because a coloured oxide layer is not the protective passive film and will corrode preferentially.
Q: Why do carbon steel carbonisation tower tubes fail so quickly in soda ash plants?
The combination of ammonia, carbon dioxide and concentrated chloride liquors is strongly corrosive to carbon steel and cast iron, and the wetted parts of carbonisation tubes, hot mother liquor coolers and crystalliser external coolers typically have a service life of no more than three years before leaking.
Q: Is titanium suitable for seawater-cooled heat exchangers?
Yes. Titanium is one of the most widely used tube materials for seawater cooling because chloride-rich, aerated water keeps the passive film intact and the metal is immune to the pitting that attacks stainless steel tubes under the same deposits and flow conditions.
Q: Which media must be kept away from titanium?
Fluoride-bearing streams, including hydrofluoric acid and fluoride-containing pickling liquors, plus strong reducing acids and dry chlorine at elevated temperature. Where any of these cannot be excluded, an alternative material or a thicker corrosion allowance has to be considered at the design stage.